Hello all, I work with low c steel (SAE 1006, 1008) from 5,5 to 14 mm inlet diameter. I am looking for new reliable efficient environment friendly (no acid)alternative for descaling wire. Currently we use bending + brushes or shot blasting.
Wire is OK for mechanical descaling but sometimes surface quality (roughness, incrusted scale...) is not good enough to ensure plating quality.
Maybe there's a new technology more efficient to eliminate surface defects on wire surface ?
Does anybody knows peeling ? Ultrasonic ? Plasma ? Laser ? technologies ?
Thanks
Wire is OK for mechanical descaling but sometimes surface quality (roughness, incrusted scale...) is not good enough to ensure plating quality.
Maybe there's a new technology more efficient to eliminate surface defects on wire surface ?
Does anybody knows peeling ? Ultrasonic ? Plasma ? Laser ? technologies ?
Thanks
Please Log in to join the conversation.
- Archived Forum Admin
- Topic Author
- Offline
- Platnium Boarder
12 years 10 months ago #918 by Archived Forum Admin
Replied by Archived Forum Admin on topic Re: Mechanical descaling
Hi Jagintoj,
we are currently mechanical descaling all our plating wires.
We use the Decalub descalng process, with a blend of sodium stripping soap that we use from Traxit Lub.
The finished wire is then blasted with water in-line to present a high gloss finish to the wire.
To achieve the gloss we use a 3-5% reduction on the last draw pass.
However, the key to ensure it's success is that we store the rod indoors. This prevents premature, accalerated rusting.
Hope this helps.
Jack
we are currently mechanical descaling all our plating wires.
We use the Decalub descalng process, with a blend of sodium stripping soap that we use from Traxit Lub.
The finished wire is then blasted with water in-line to present a high gloss finish to the wire.
To achieve the gloss we use a 3-5% reduction on the last draw pass.
However, the key to ensure it's success is that we store the rod indoors. This prevents premature, accalerated rusting.